Active Screen Plasma Nitriding – An Efficient, New Plasma Nitriding Technology
by Pierre Collignon
Jean Georges
Christian Kunz
January 6, 2012
Active
screen plasma nitriding technology (ASPN) is a new industrial solution that
enjoys all the advantages of traditional plasma nitriding but does not have its
inconveniences. Different-size parts can be treated in the same batch. It also
offers the possibility of oxynitriding and nitriding of stainless steels. ASPN
is also called “easy nitriding” because it does not require highly skilled
operators.
Nitriding,
which is a nitrogen diffusion technique, has the great advantage of using
relatively low temperatures (450-590°C/850-1100°F), allowing it to be utilized
on most mechanically finished parts.
Development of Nitriding Technologies
|
|
| Fig. 1. Active
screen surrounding the parts |
|
Several techniques have been developed to industrially
achieve the nitriding process over the last century.
Gaseous Nitriding (1910-1920)
This process using
ammonia (NH 3) is still the most commonly used technology for
nitriding today. Though the equipment is not expensive, it comes with very high
running cost due to high energy and gas consumption. In addition, it does not
allow a good control of the structure.
Salt-Bath Nitriding (1940-1950)
Its use today is decreasing, and in many countries it is
not even allowed anymore due to the environmental impact of the chemicals and
the emissions. Its high running costs stem from the energy consumption and
expenses to clean the parts.
Plasma Nitriding (1965-1975)
First developed using
cold-wall furnaces, plasma nitriding has significant advantages: very low
running costs (reduced consumption of energy and gases); controllable;
optimized structure and layers; and nitriding of stainless steels. Plasma
nitriding is totally safe and has no poisonous gas emissions and no negative
environmental impact. However, conventional plasma nitriding has a number of
well-known difficulties, including the direct application of plasma on the
parts to be treated, the risk of arcing, hollow cathodes, white layers,
non-homogenous batch temperature and the impossibility to mix parts of
different geometries in the chamber. Thus, it requires well-trained, highly
skilled operators.
In the early
1980s, plasma nitriding became much easier thanks to the development of pulsed
power supplies and automatic gas-flow control. All these innovations using
hot-wall furnaces were first presented by co-author Pierre Collignon in 1982.
Within 10 years, this new type of furnace and process became the industrial
standard. However, some inconveniences exist to this day with hot-wall furnaces
(e.g., temperature homogeneity, limited control of metallurgical structure, expensive
equipment and maintenance).
Active Screen Plasma Nitriding
|
|
| Fig. 2. Commercial
ASPN furnace
(Courtesy of Plasma Metal/PD2i) |
|
ASPN is a technology that has been developed and
commercially used in recent years. There is finally a technology that resolves
the difficulties of conventional plasma nitriding.
ASPN Technology: How it Works
With the active screen, the plasma is no longer applied to
the workload but rather to a metallic screen that surrounds the parts (Fig. 1).
The parts to be nitrided are either placed on a floating potential or a light
bias is applied. Plasma forms on the screen and not on the parts under these
conditions. The screen heats up quickly, which heats the workload by radiation.
In this way, the whole workload heats up to the correct nitriding temperature.
The screen also supplies the active species, which quickly diffuses into the
materials to form the expected nitrided layers. The temperature control is
achieved by regulating the plasma power on the active screen. Reactive gases (N 2,
H 2, C xH y) are pumped from the middle of the
chamber and flow through the active screen. This assures a gentle flow of
reactive species over the entire workload.
|
|
| Fig. 3. Mixed
batches can be treated |
|
Treatment of the Parts
Because the parts are no longer directly exposed to the
glow, the problems related to conventional plasma nitriding are eliminated (arcing,
hollow cathodes, temperature heterogeneity, etc.). Degreasing with chloride
solvents or ultrasonic-assisted cleaning for complicated parts is no longer
necessary. Simply degreasing by washing (steam cleaning) is sufficient.
Homogenous batch loading is no longer required. Therefore, parts with different
shapes, geometries and steel types can be treated in the same batch (Fig. 3).
The space between parts can be reduced to increase the load density. The entire
vacuum chamber can be used due to the excellent temperature homogeneity. In
contrast, only 50% of the available chamber volume can be used most of the time
with DC plasma-nitriding equipment.
Metallurgical Structures
Similar to the classic processes, the diffusion layer
thickness as well as the hardness depend primarily on the steel used. The
hardness obtained typically varies from 600 to 1,200 Vickers, and layer depths
vary from 0.01-0.3mm. In addition, ASPN delivers essentially the same
structures as conventional DC plasma nitriding.
|
|
| Fig. 4. Hardness and
case depth for H13 (left) and D2 (right) tool steels treated at 500°C
(932˚F)with ASPN |
|
ASPN of Tool Steel
Tool steels are nitrided to improve their surface hardness, scratch
resistance and wear resistance. To investigate the response of tool steel
toward ASPN, H13 (0.35C, 1.5Mo, 5Cr, 1V) and D2 (1.5C, 1.0Mo, 12Cr) steels were
nitrided at 500°C for 5-40 hours. Figure 4 shows that both tool steels were hardened
considerably after ASPN treatment. The maximum hardness in the nitrided case
was more than 1,000 HV. The case depth varied from 100-300 µm, depending on
treatment time. Containing a higher amount of chromium, D2 steel shows higher
case hardness but shallower case depth than H13.
|
|
| Fig. 5. Optical (a)
and SEM (b) microstructures of ASPN 316 steel |
|
ASPN of Stainless Steels
It is possible to make low-temperature treatments
(350-450°C) on stainless steels due to good temperature homogeneity achieved
with ASPN. The complete absence of precipitates, nitrides and carbides allows
the steel to remain stainless while increasing its wear resistance by a factor
of 100 (Fig. 5). ASPN is applied to parts in nuclear, medical, aerospace, food
and chemical applications.
Nitriding + Post Oxidation
With the active screen, the nitriding can be immediately
followed by a plasma-assisted oxidizing process of approximately 30 minutes.
This increases the corrosion resistance to the same level as obtained with
conventional salt-bath processes. The potential applications are numerous
(e.g., tool holders or automotive components like steering knuckles).
ASPN of Polymeric Materials
The ASPN technique has been used to modify the surface of several
polymeric materials, including ultrahigh molecular-weight polyethylene
(UHMWPE), polypropylene and polyoxymethylene (POM). It has been shown that ASPN can effectively modify the surface chemical
composition and bond structure. The ASPN-treated polymers
have considerably improved hardness, elastic modulus, creep resistance, scratch
resistance and wear resistance.
ASPN - An Economical Trump
Significant productivity gains are achieved with ASPN due
to simplified load buildup, less complex degreasing procedures and higher load
density. Furthermore, ASPN enables exceptional savings on consumables and
energy (see Sidebar 1). For example, savings on electricity were 15% and 95% on
gases for a 1-ton load of forging dies of X40CrMoV5 steel.
Conclusion
ASPN is a recently developed technology that provides
solutions to many wear-resistance problems. It resolves the various inconveniences
of conventional DC plasma nitriding while maintaining its numerous advantages.
Metallurgically, the obtained structures are optimal and may be adapted to any
need. They are fully reproducible since every parameter is piloted by automatic
controls. The treatments are mostly done on steel but can be extended to other
materials (Ti, polymers and powders). High-density loads, reduced energy
consumption and reduced gas consumption make ASPN an economically competitive
process. It does not produce any dangerous or toxic products or wastes, and it
allows working in fully secure conditions with complete respect to the
environment. IH
For more information:
Contact Dr. Christian Kunz, president, PD2i North America, 12816 Stahl
Drive, Knoxville, TN 37934; tel: 865-321-3932; e-mail: christian.kunz@pd2i.com;
web: www.pd2i.com
SIDEBAR 1
ASPN – Lowest Running-Cost
Technology
for Nitriding
-
Very low gas consumption
-
Low energy consumption due to efficient heating
- Short cycle times
- Very low spare-parts consumption
ASPN – An Environmentally
Friendly Technology
- No poisonous emissions
- No environmentally hazardous materials
- Safe for operators
SIDEBAR 2
Typical Applications
- Components (crankshafts, camshafts, gears, pistons, valves, cylinders,
valve springs, shafts, spindle, sliding rails, pump cylinders)
- All types of hot-forging dies
- All types of extrusion dies
- Sheet-metal forming punches and dies
- Rolling dies
- Aluminum die-casting molds
- Plastic extruder screws, molds for injection molding
- Tool holders and taps
|